Our research focuses on the development of near- to mid-infrared photodetectors using lead telluride (PbTe) and cadmium telluride (CdTe) semiconductors in the active region [1,2]. PbTe is a direct narrow-bandgap material (0.32 eV at 300 K), which enables the formation of quantum wells and quantum dots that are sensitive to infrared radiation at room temperature. In contrast, CdTe also has a direct, but wider bandgap (1.49 eV at 300 K), making it sensitive to the visible spectral range. In our design, CdTe serves as a barrier material for the PbTe layers. The performance of these photodetectors, particularly their detectivity, can be tuned by adjusting structural parameters such as the thickness and number of layers. In this work, we seek to identify the optimal growth temperature ranges for the active layers, along with the optimal post-growth annealing temperature and time, to enhance device detectivity.
To study the effect of growth temperature dependence, we fabricated 12 structures consisting of six alternating PbTe/CdTe layers divided in two series. These structures were grown using molecular beam epitaxy (MBE) with elemental sources of Cd, Pb, and Te on semi-insulating GaAs (100) substrates. The first series of structures has 25 nm-thick PbTe layers and varies in substrate temperature from 230°C to 350°C, while the second series was grown at 350°C and varies in PbTe layer thickness from 25 nm to 47 nm. To investigate the effects of post-deposition annealing, we analysed another photoresistor structure consisting of four alternating PbTe/CdTe layers, which was cut into several dozen samples measuring 3 × 3 mm2. These samples were annealed at temperatures from 150°C to 300°C for 5 to 20 minutes, either with or without indium contacts present during annealing process.
We performed basic current–voltage (I–V) and spectral response (SR) measurements in the near- to mid-infrared range for each sample. We observed that detectors grown at different substrate temperatures exhibit higher detectivity with increasing substrate temperature, with the structure grown at 290°C reaching the maximum detectivity. Other detectors from this series show a decrease in detectivity with further increases in substrate
temperature. Detectors from the series with varying PbTe layer thicknesses show that longer PbTe growth, at around 350°C substrate temperature, leads to the formation of thicker PbTe layers instead of quantum dots, and this also improves the detectivity of the grown detectors. The post-growth annealing results show that the presence of indium contacts during this process significantly increases device detectivity over time, by up to a factor of 6 after 10 minutes at 150°C compared to non-annealed detectors. Samples without pre-annealed indium contacts exhibit overall lower detectivity compared to samples with indium contacts, especially for detectors annealed at temperatures above 240 °C, where their detectivity was lower than that of devices without any annealing. This leads to the conclusion that, during annealing, indium from the contacts diffuses through the PbTe/CdTe layers and enhances the collection of photogenerated carriers, thereby improving total detector detectivity. This effect is observed even for samples annealed at around 150°C, where indium does not melt and its diffusion is lower than at higher temperatures.
[1] S. Chusnutdinow, S. Schreyeck, S. Kret, A. Kazakov, and G. Karczewski, Appl. Phys. Lett. 177, 072102 (2020).
[2] J. M. Gluch, M. Szot, S. Chusnutdinow and G. Karczewski, Appl. Phys. Lett. 126, 121101 (2025).
The research in Poland was supported by the National Science Centre through the Grant No.2021/41/B/ST3/03651 and partially supported by the “MagTop” project (FENG.02.01-IP.05-0028/23) carried out within the “International Research Agendas” programme of the Foundation for Polish Science co-financed by the European Funds for Smart Economy 2021-2027 (FENG).